收藏词条 编辑词条 日本标准片状石墨型奥氏体铸铁的牌号、抗拉强度与化学成分(质量分数)(%)
牌 号 C Si Mn Cr Ni Cu 抗拉强度 σb≥/Mpa FCA-NiMn137 ≤3.0 1.5~3.0 6.0~7.0 ≤0.2 12.0~14.0 ≤0.5 140 FCA-NiCuCr1563 ≤3.0 1.0~2.8 0.5~1.5 1.0~2.5 13.5~17.5 5.5~7.5 170 FCA-NiCuCr1563 ≤3.0 1.0~2.8 0.5~1.5 2.5~3.5 13.5~17.5 5.5~7.5 190 F190CA-NiCr202 ≤3.0 1.0~2.8 0.5~1.5 1.0~2.5 18.0~22.0 ≤0.5 170 FCA-NiCr203 ≤3.0 1.0~2.8 0.5~1.5 2.5~3.5 18.0~22.0 ≤0.5 190 FCA-NiSiCr2053 ≤2.5 4.5~5.5 0.5~1.5 1.5~4.5 18.0~22.0 ≤0.5 190 FCA-NiCr303 ≤2.5 1.0~2.0 0.5~1.5 2.5~3.5 28.0~32.0 ≤0.5 190 FCA-NiSiCr3055 ≤2.5 5.0~6.0 0.5~1.5 4.5~5.5 29.0~32.0 ≤0.5 170 FCA-Ni35 ≤2.5 1.0~2.0 0.5~1.5 ≤0.2 34.0~36.0 ≤0.5 120